Steel For Forming

Hot-rolled steel for cold forming is used for bending and deep drawing.
Jeavons Coil’s forming grades offer consistency for reliable processing and low carbon content for excellent welding performance.

DD11

DD12

DD13

DD14

Mechanical Properties

EN 10111:2008 Gauge DD11
Yield strength ReL (N/mm2) 1.5 ≤ t < 2 170-360
Yield strength ReL (N/mm2) 2 ≤ t < 11 170-340
Max. tensile strength Rm (N/mm2) 440
Min. Elongation % 1.5 ≤ t < 2 23
Min. Elongation % 2 ≤ t < 3 24
Min. Elongation % 3 ≤ t < 11 28
Min. bend test diameter 1t

Chemical  Composition

EN 10111: 2008 DD11
C 0.12 Max.
Mn 0.60 Max.
P 0.045 Max.
S 0.045 Max.

Mechanical Properties

EN 10111: 2008 Gauge DD12
Yield strength ReL (N/mm2) 1.5 ≤ t < 2 170 – 340
Yield strength ReL (N/mm2) 2 ≤ t < 11 170 – 320
Max. tensile strength Rm (N/mm2) 420
Min. Elongation % 1.5 ≤ t < 2 25
Min. Elongation % 2 ≤ t < 3 26
Min. Elongation % 3 ≤ t < 11 30
Min. bend test diameter 0t

Chemical Composition

EN 10111: 2008 DD12
C 0.10 Max.
Mn 0.45 Max.
P 0.035 Max.
S 0.035 Max.

Mechanical Properties

EN 10111: 2008 Gauge DD13
Yield strength ReL (N/mm2) 1.5 ≤ t < 2 170 – 330
Yield strength ReL (N/mm2) 1.5 ≤ t < 2 170 – 310
Max. tensile strength Rm (N/mm2) 400
Min. Elongation % 1.5 ≤ t < 2 28
Min. Elongation % 2 ≤ t < 3 29
Min. Elongation % 3 ≤ t < 11 33
Min. bend test diameter 0t

Chemical Compostion

EN 10111: 2008 DD13
C 0.08 Max.
Mn 0.4 Max.
P 0.03 Max.
S 0.03 Max.

Mechanical Properties

EN 10111: 2008 Gauge DD14
Yield strength ReL (N/mm2) 1.5 ≤ t < 2 170 – 310
Yield strength ReL (N/mm2) 2 ≤ t < 11 170 – 290
Max. tensile strength Rm (N/mm2) 380
Min. Elongation % 1.5 ≤ t < 2 31
Min. Elongation % 2 ≤ t < 3 32
Min. Elongation % 3 ≤ t < 11 36
Min. bend test diameter 0t

Chemical Composition

EN 10111: 2008 DD14
C 0.08 Max.
Mn 0.35 Max.
P 0.025 Max.
S 0.025 Max.